Processing ATABOND resins

The right temperature for every zone.

Recommended extrusion temperatures, shutdown, purging and storage for PE-based and PP-based grades.

Recommended temperatures

Maximum temperature: 280-300 °C

PE-based and PP-based grades side by side

ZonePE-based, °CPP-based, °C
Zone 1170-200200-230
Zone 2170-200200-230
Zone 3200-230200-250
Zone 4200-230200-250
Adapter200-230200-250
Die200-230200-250
Melt temperature200-230200-240
Maximum temperature280-300

Temperatures above the upper limit or long residence times of molten resin may lead to decomposition of the polymer. Decomposition products may be carbon dioxide, carbon monoxide, hydrocarbons and water.

Shutdown

  • Less than 2 hours: screw rotation can be stopped while maintaining temperature.
  • More than 2 hours: purge out and shut down in accordance with common procedure.

Purging

For a permanent shutdown, purge with PE (MFI 1): PE-based 200-230 °C, PP-based 200-240 °C.

Storage

ATABOND resins are supplied as small, free-flowing pellets and can be handled with commercially available equipment.

  • Store and transport at a temperature below 50 °C
  • Protect from moisture
  • Keep containers tightly sealed in a dry, cool and well-ventilated place

Why moisture matters: in the presence of moisture the anhydride group converts to its acid form. US 9902882 B2

What are you bonding?

Choose your structure. The right ATABOND follows, with a sample and a quotation.

Start a request